TL;DR: Insulation paper wrinkles during winding for five reasons: wrong web tension, moisture-driven dimensional change, paper quality defects, machine misalignment, and conductor geometry forcing paper around tight bends. Most wrinkling is fixed by tension control, 40–60% RH shop climate, and roll alignment — not by changing paper supplier.
Insulation paper wrinkling is the formation of folds, ridges, or wavy edges in paper layers while winding transformer coils. Wrinkles create air pockets that lower dielectric strength, add uneven radial build that distorts winding geometry, and can crack the paper at fold lines — a weak point for partial discharge. The five root causes are tension errors, moisture imbalance, paper defects, machine misalignment, and bend geometry, and each has a distinct wrinkle signature you can diagnose on the shop floor.
This guide maps each wrinkle pattern to its cause, gives a troubleshooting table and a prevention checklist, and clarifies when the answer is not tighter process control but a different paper — crepe instead of flat kraft. SIDA supplies both, with batch-level tensile and moisture documentation on every lot.
What Are the Five Root Causes of Wrinkling During Winding?

{{IMG1}}
1. Wrong web tension. Too little tension and layers go down slack, buckling under the next layer. Too much and the paper stretches elastically, then contracts after winding — producing wrinkles hours later. Tension must also be uniform across the web width; a roll running 10% tighter on one edge produces diagonal wrinkles marching across the layer. Verify actual tension with a hand-held web tension meter, not the machine dial: measure at the roll and again just before the winding point, because friction across guide rollers drops tension along the path.
2. Moisture imbalance. Cellulose expands and contracts with humidity, mostly across the grain — a reel moving from 70% RH storage into a 45% RH winding shop shrinks enough across its width to slacken the web mid-run. Paper stored damp develops expanded, wavy edges (“dishing”); paper dried hard and then left open in humid air curls. This is the same physics covered in our insulation paper drying and moisture control guide — moisture moves paper dimensions before it ever affects dielectric properties.
3. Paper quality defects. Uneven caliper across the reel, poor formation, excessive curl, telescoped rolls, or low tensile strength all show up as wrinkling under otherwise correct settings. Delivered moisture above 8% is itself a defect claim. Verify against the CoA — our sample testing protocol covers incoming checks.
4. Machine misalignment. A mandrel not parallel to the guide rollers, worn bearings letting the roll oscillate, an eccentric cardboard core, or uneven pressure roller contact all steer the web sideways. Steering under tension is wrinkling.
5. Conductor geometry. Flat kraft paper cannot wrap a tight corner or irregular lead exit without folding — it has almost no stretch. Forcing it around geometry is not a defect; it is the wrong material choice, covered in the crepe vs. flat section below.
How Do You Diagnose the Cause from the Wrinkle Pattern?
The wrinkle pattern is diagnostic evidence. Match what you see on the winding to this table before changing anything:
| Wrinkle Pattern | Most Likely Cause | First Fix to Try |
|---|---|---|
| Loose, random folds across whole layer | Tension too low | Raise tension gradually; check dancer/brake function |
| Diagonal wrinkles in a consistent direction | One-sided tension / misalignment | Check roll parallelism and mandrel level |
| Wavy edges, center tight | Moisture pickup at edges (dishing) | Check storage RH; acclimatize rolls 24–48 h in shop |
| Wrinkles appear hours after winding | Over-tension stretch recovery | Reduce tension; verify with strip test |
| Same position on every reel | Paper defect (caliper, curl) | Measure thickness profile; claim against CoA |
| Folds only at corners or lead exits | Geometry exceeds paper stretch | Switch to crepe paper for those zones |
What Is on the Prevention Checklist?

{{IMG2}}
Climate: hold the winding shop at 40–60% RH and 18–25°C. Acclimatize sealed rolls in the shop for 24–48 hours before opening — a cold roll opened in warm humid air condenses moisture on its outer layers.
Tension: set web tension by paper thickness and width, using the machine’s closed-loop control where available; as a starting range, thin cable papers run a few N/cm of width, heavier presspapers proportionally more. Log settings per material lot so a good recipe is repeatable.
Machine: verify mandrel-to-roller parallelism on a schedule, not after defects appear. Replace damaged cores, keep guide rollers clean and free-spinning, and confirm pressure roller contact is even across the width. Ramp winding speed up gradually at layer starts — a hard start jerks the web and leaves a wrinkle exactly where the layer begins.
Material handling: store rolls on end, never on their side; keep factory PE wrapping on until use; follow FIFO. Roll handling damage (edge nicks, telescoping) becomes winding defects downstream.
Orientation: paper is stronger and stiffer in the machine direction — the facing-direction and MD/CD logic in our kraft paper facing guide applies to winding setup as well.
When Is the Answer Crepe Paper Instead of Flat Kraft?

{{IMG3}}
If wrinkles appear only where paper must follow curved or irregular shapes — lead exits, tap changers, coil ends, corner bends — the fix is material, not process. Crepe paper is creped during manufacture to give elongation that lets it conform to contours flat kraft cannot follow: standard crepe grades offer around 50% stretch, high-elongation grades 100% or more, and micro-crepe variants trade some stretch for a smoother surface finish. Our crepe paper complete technical guide covers grades, elongation ratings, and where each is used.
Rule of thumb: flat kraft or pressboard for straight layer and barrier insulation; crepe paper wherever the path bends. Diamond-dotted paper (DDP) adds epoxy dots for layer bonding in distribution windings. High-voltage layer design has additional constraints — our 220kV+ paper specification guide covers thickness grading, and instrument transformers add their own rules in the CT/VT insulation paper guide.
FAQ
Is wrinkling always a paper quality problem? No — in our experience most winding wrinkles trace to tension settings, climate, or machine alignment. Paper defects (caliper variation, curl, telescoped reels) are real but show a consistent pattern repeating at the same reel position. Diagnose the pattern before claiming material.
Does a wrinkle actually hurt the transformer? Yes. A fold creates a local air void with lower partial discharge inception voltage, doubles the insulation thickness unevenly so winding geometry drifts, and the fold line itself is mechanically cracked cellulose. Cosmetic wrinkles on outer layers matter less; wrinkles buried in the winding matter a lot.
What humidity should a winding shop maintain? 40–60% RH and 18–25°C is the widely used window — humid enough that paper stays flexible, dry enough that dimensional change stays small. Acclimatize rolls in the shop 24–48 hours before opening.
Does crepe paper wrinkle during winding? Crepe paper conforms instead of folding — that is its purpose. But it still wrinkles from wrong tension or misalignment, and its higher elongation makes tension control more sensitive, not less.
Can I still use a reel that arrived with wavy edges? Measure first. Edge waviness from moisture (dishing) sometimes relaxes after acclimatization; caliper-driven waviness does not. If the wave persists after 48 hours at shop conditions, document and claim it against the lot CoA.
What tension should I use for a given paper thickness? There is no universal number — it depends on width, thickness, machine, and winding speed. Start from your machine maker’s data or the paper supplier’s recommendation, verify with a tension meter at the winding point, and record the working recipe per lot. A wrinkle-free trial layer at low speed is worth more than any table.
Can wrinkled layers be repaired after winding? Only by unwinding and rewinding them — and only before vacuum drying and oil impregnation. Once a coil is dried and impregnated, wrinkles are permanent. That is why the troubleshooting table above pays for itself: catching the pattern on the first bad layer saves a complete rewind.
Get Winding-Proven Paper from SIDA
Consistent winding starts with consistent material: uniform caliper, documented moisture, and tensile values on every CoA. SIDA’s Guangxin mills produce cable paper, crepe paper, and pressboard with batch traceability, and our team helps you match grade and width to your winding process — see the full range in our insulation materials guide.
Describe your winding problem or send your specification through the contact form, or reach Jessie Feng directly via WhatsApp +86-15958243831 / jessie.feng@sidanm.com.